37 grades · 7 cast · 30 wrought
High-Copper Alloys (Beryllium / Chromium / Zirconium Copper)
Heat-treatable copper with high strength and conductivity: welding electrodes, springs, connectors. 37 grades across USA, European, German, British, Japanese and Chinese standards — each with its own datasheet and cross-reference.
37 of 37 grades
| Grade | Name | System | Form | Composition |
|---|---|---|---|---|
| C81500● data | Chromium copper | USA · UNS | Cast | Cr 0.4–1.5, Cu rem |
| C82000● data | Beryllium copper 10C | USA · UNS | Cast | Be 0.45–0.8, Co 2.4–2.7, Cu rem |
| C82500● data | Beryllium copper 20C | USA · UNS | Cast | Be 1.9–2.25, Co 0.35–0.7, Si 0.2–0.35, Cu rem |
| CC140C● data | CuCr1-C | Europe · EN 1982:2017 | Cast | Cr 0.4–1.2, Cu rem (precipitation hardened) |
| 2.1292● data | G-CuCrF35 | Germany · DIN 17655 | Cast | Cr 0.4–1.2, Cu rem |
| CC1-TF● data | CC1-TF | UK · BS 1400:1985 | Cast | Cr 0.6–1.2, Cu rem (solution + precipitation treated) |
| HCC1● data | HCC1 | UK · BS 1400:1985 | Cast | Cu ≥ 99.9 (high conductivity) |
| C14500● data | Tellurium copper | USA · UNS / ASTM B301, B124 | Wrought | Cu rem, Te 0.4-0.7, P 0.004-0.012 |
| CW118C● data | CuTeP | Europe · EN 1412 numbering | Wrought | Cu rem, Te 0.4-0.7, P 0.004-0.012 |
| 2.1546● data | CuTeP | Germany · DIN 17660 / 17662 / 17663 / 17664 / 1766 | Wrought | Cu rem, Te 0.4-0.7, P 0.004-0.012 |
| C109● data | Tellurium copper | UK · BS 2870-2875 | Wrought | Cu rem, Te 0.4-0.7, P 0.004-0.012 |
| C15000● data | Zirconium copper | USA · UNS / ASTM B422 | Wrought | Cu rem, Zr 0.10-0.20 |
| CW120C● data | CuZr | Europe · EN 1412 numbering | Wrought | Cu rem, Zr 0.10-0.20 |
| 2.1580● data | CuZr | Germany · DIN 17660 / 17662 / 17663 / 17664 / 1766 | Wrought | Cu rem, Zr 0.10-0.20 |
| C18200● data | Chromium copper | USA · UNS / ASTM B224 | Wrought | Cu rem, Cr 0.5-1.2 |
| CW105C● data | CuCr1 | Europe · EN 1412 numbering | Wrought | Cu rem, Cr 0.5-1.2 |
| 2.1291● data | CuCr | Germany · DIN 17660 / 17662 / 17663 / 17664 / 1766 | Wrought | Cu rem, Cr 0.5-1.2 |
| CC101● data | Chromium copper | UK · BS 2870-2875 | Wrought | Cu rem, Cr 0.5-1.2 |
| C18150● data | Chromium-zirconium copper | USA · UNS / ASTM B224 | Wrought | Cu rem, Cr 0.5-1.2, Zr 0.03-0.3 |
| CW106C● data | CuCr1Zr | Europe · EN 1412 numbering | Wrought | Cu rem, Cr 0.5-1.2, Zr 0.03-0.3 |
| 2.1293● data | CuCrZr | Germany · DIN 17660 / 17662 / 17663 / 17664 / 1766 | Wrought | Cu rem, Cr 0.5-1.2, Zr 0.03-0.3 |
| CC102● data | Chromium-zirconium copper | UK · BS 2870-2875 | Wrought | Cu rem, Cr 0.5-1.2, Zr 0.03-0.3 |
| C17200● data | Beryllium copper (2 Be) - alloy 25 | USA · UNS / ASTM B194, B196, B197 | Wrought | Cu rem, Be 1.8-2.0, Co+Ni >= 0.2 |
| CW101C● data | CuBe2 | Europe · EN 1412 numbering | Wrought | Cu rem, Be 1.8-2.0, Co+Ni >= 0.2 |
| 2.1247● data | CuBe2 | Germany · DIN 17660 / 17662 / 17663 / 17664 / 1766 | Wrought | Cu rem, Be 1.8-2.0, Co+Ni >= 0.2 |
| CB101● data | Beryllium copper (2 Be) - alloy 25 | UK · BS 2870-2875 | Wrought | Cu rem, Be 1.8-2.0, Co+Ni >= 0.2 |
| C1720● data | Beryllium copper (2 Be) - alloy 25 | Japan · JIS H 3100 / H 3250 / H 3300 | Wrought | Cu rem, Be 1.8-2.0, Co+Ni >= 0.2 |
| C17500● data | Cobalt-beryllium copper (Class 3) | USA · UNS / ASTM B441 | Wrought | Cu rem, Co 2.4-2.7, Be 0.4-0.7 |
| CW104C● data | CuCo2Be | Europe · EN 1412 numbering | Wrought | Cu rem, Co 2.4-2.7, Be 0.4-0.7 |
| 2.1285● data | CuCo2Be | Germany · DIN 17660 / 17662 / 17663 / 17664 / 1766 | Wrought | Cu rem, Co 2.4-2.7, Be 0.4-0.7 |
| C112● data | Cobalt-beryllium copper (Class 3) | UK · BS 2870-2875 | Wrought | Cu rem, Co 2.4-2.7, Be 0.4-0.7 |
| C17510● data | Nickel-beryllium copper (Class 3) | USA · UNS / ASTM B441, B534 | Wrought | Cu rem, Ni 1.4-2.2, Be 0.2-0.6 |
| CW110C● data | CuNi2Be | Europe · EN 1412 numbering | Wrought | Cu rem, Ni 1.4-2.2, Be 0.2-0.6 |
| 2.0850● data | CuNi2Be | Germany · DIN 17660 / 17662 / 17663 / 17664 / 1766 | Wrought | Cu rem, Ni 1.4-2.2, Be 0.2-0.6 |
| C64700● data | Copper-nickel-silicon (Corson) 2Ni | USA · UNS / ASTM B411, B412 | Wrought | Cu rem, Ni 1.6-2.2, Si 0.4-0.8 |
| CW111C● data | CuNi2Si | Europe · EN 1412 numbering | Wrought | Cu rem, Ni 1.6-2.5, Si 0.4-0.8 |
| 2.0855● data | CuNi2Si | Germany · DIN 17660 / 17662 / 17663 / 17664 / 1766 | Wrought | Cu rem, Ni 1.6-2.5, Si 0.4-0.8 |
Overview
High-copper alloys are coppers with small additions — usually under 3% in total — of chromium, zirconium, beryllium, cobalt, nickel, silicon or tellurium that make the metal much stronger, harder or easier to machine while keeping most of copper's electrical and thermal conductivity. Most of them are precipitation-hardening: they are solution treated and then aged so that tiny particles of the alloying element form inside the copper and block deformation. The result is a family of materials that sits between pure copper (high conductivity, low strength) and bronzes (high strength, low conductivity).
This guide covers the cast grades in the library (chromium copper C81500 / CC140C, beryllium coppers C82000 and C82500) and the wrought grades most often machined into parts (tellurium copper C14500, zirconium copper C15000, chromium copper C18200, chromium-zirconium copper C18150, beryllium coppers C17200, C17500 and C17510, and the Corson alloy C64700), with their EN, DIN, BS and JIS equivalents.
Why add anything to copper?
Pure copper conducts superbly but is soft, and it loses what strength it has when heated: an annealed copper electrode or contact deforms under load and softens further at a few hundred degrees. Adding a solid-solution element such as zinc or tin (as in brass and bronze) makes copper stronger but destroys conductivity. High-copper alloys solve the problem differently. Elements such as chromium, zirconium and beryllium dissolve in copper at high temperature but not at room temperature. After a solution treatment and quench, an ageing treatment precipitates them as fine particles. The copper matrix around the particles becomes almost pure again — so conductivity recovers — while the particles give strength and resistance to softening.
The metallurgy in plain words
Chromium copper (C18200, C81500, CC140C)
About 0.5–1.2% chromium. After ageing it typically combines roughly 75–85% IACS conductivity with strength several times that of annealed copper. It keeps its hardness at elevated temperatures far better than pure copper, which is why it is the standard material for resistance-welding electrodes, holders and current-carrying parts that run hot. The cast version (C81500 in the USA, CC140C / CuCr1-C in EN 1982, CC1-TF in BS) is used for welding-machine parts, electrode holders, tuyeres and other heavy conductor castings.
Chromium-zirconium copper (C18150, CW106C)
A small zirconium addition to chromium copper raises the softening temperature further and improves fatigue and creep resistance. It is the common choice for spot-welding caps and seam-welding wheels (RWMA Class 2), continuous-casting mold parts and high-temperature conductors.
Zirconium copper (C15000, CW120C)
About 0.1–0.2% zirconium. Strength is lower than chromium copper but conductivity is higher (typically around 90% IACS), and resistance to softening is good. Used for commutators, electrodes for some materials and high-conductivity parts that see moderate heat.
Tellurium copper (C14500, CW118C)
About 0.4–0.7% tellurium plus a trace of phosphorus. Tellurium forms tiny particles that break chips during machining, so the material machines far more easily than pure copper while still conducting at roughly 90% IACS. It is not a strength alloy — it is chosen for intricate machined conductors such as terminals, connector pins, plasma-torch tips and electrical fittings.
Beryllium copper (C17200, C17500, C17510, C82000, C82500)
The strongest copper alloys. The high-strength grades (C17200 wrought, C82500 cast, about 2% beryllium) can be aged to strengths comparable with many steels — typically well above 1,000 MPa for wrought C17200 — with good spring properties, wear resistance and non-sparking behavior, but conductivity is only around 20–25% IACS. The high-conductivity grades (C17500 with cobalt, C17510 with nickel, cast C82000, all with about 0.2–0.8% beryllium) trade some strength for conductivity of roughly 45–60% IACS and are used as RWMA Class 3 electrode materials and for heavy-duty current-carrying springs and contacts.
Corson copper (C64700, CW111C)
Nickel and silicon (about 2% Ni, 0.5% Si) precipitate as nickel silicide. This beryllium-free alloy gives good strength, moderate conductivity (typically around 40% IACS) and good resistance to stress relaxation, and is used for connectors, lead frames, springs and welding parts.
Grades in this category compared
| Grade (USA) | EN | Form | Main additions | Typical conductivity | Main strength level | Typical use |
|---|---|---|---|---|---|---|
| C14500 | CW118C CuTeP | Wrought | Te 0.4–0.7 | About 90% IACS | Low (like copper) | Free-machining conductors |
| C15000 | CW120C CuZr | Wrought | Zr 0.1–0.2 | About 85–93% IACS | Moderate | Hot conductors, commutators |
| C18200 | CW105C CuCr1 | Wrought | Cr 0.5–1.2 | About 75–85% IACS | Moderate–high | Welding electrodes, holders |
| C18150 | CW106C CuCr1Zr | Wrought | Cr + Zr | About 75–85% IACS | Moderate–high, best at temperature | Spot-welding caps, mold parts |
| C81500 | CC140C CuCr1-C | Cast | Cr 0.4–1.5 | Typically about 80% IACS (heat treated) | Moderate | Cast electrode holders, conductor castings |
| C17500 / C17510 | CW104C / CW110C | Wrought | Be 0.2–0.7 + Co or Ni | About 45–60% IACS | High | RWMA Class 3 electrodes, contacts |
| C82000 | — | Cast | Be 0.45–0.8, Co 2.4–2.7 | Typically about 45% IACS | High | Cast welding parts, contacts |
| C17200 | CW101C CuBe2 | Wrought | Be 1.8–2.0 | About 20–25% IACS | Very high | Springs, non-sparking tools, bushings |
| C82500 | — | Cast | Be 1.9–2.25 | Typically about 20% IACS | Very high | Plastic-mold inserts, cast high-strength parts |
| C64700 | CW111C CuNi2Si | Wrought | Ni 1.6–2.5, Si 0.4–0.8 | About 35–45% IACS | High | Connectors, springs |
All values are typical ranges for the heat-treated (aged) condition from published Copper Development Association and producer data. Actual values depend on temper and heat treatment; the governing specification and the material test certificate define what you receive.
Heat treatment: the step that makes the alloy
For chromium, chromium-zirconium, zirconium, beryllium and Corson coppers, the properties you pay for exist only after correct heat treatment:
- Solution treatment. The part is heated close to 1,000 °C (exact temperature depends on the grade) so the alloying element dissolves, then quenched rapidly in water.
- Machining (optional at this stage). In the solution-treated condition the alloy is relatively soft and machines more easily.
- Ageing (precipitation hardening). A lower-temperature soak, typically a few hundred degrees for a few hours, precipitates the strengthening particles and restores conductivity.
For castings this means the drawing must state the required condition — for example "solution treated and aged" — and the hardness or conductivity to be achieved. A chromium-copper casting supplied as-cast will have much lower strength and conductivity than the same part properly heat treated.
Casting methods that suit high-copper alloys
- Sand casting — for chromium-copper electrode holders, transformer and furnace conductor castings, and beryllium-copper parts in low to medium quantities.
- Investment casting — for small, detailed beryllium-copper and chromium-copper parts, including plastic-injection mold components.
- Centrifugal and continuous casting — for rings, sleeves and bar stock to be machined.
Chromium and zirconium oxidize readily in the melt, so these alloys need careful melting under cover and controlled pouring. Many smaller conductor parts are therefore machined from wrought bar instead, and Conex machines both routes in-house.
Applications by industry
| Industry | Parts | Usual grades |
|---|---|---|
| Resistance welding | Electrode caps, holders, shanks, seam-welding wheels, transformer pads | C18150, C18200, C17510, C81500 |
| Steel & continuous casting | Mold plates and tubes, tuyeres, lances | C18150, C18200, C81500 |
| Electrical & switchgear | Contact fingers, current-carrying springs, terminals | C17510, C14500, C18200 |
| Oil & gas, mining | Non-sparking tools, bushings, wear parts | C17200, C82500 |
| Plastics tooling | Mold inserts and cores for fast cooling | C82500, C17200, C17510 |
| Electronics & connectors | Springs, connector contacts | C17200, C64700 |
How to choose between grades
- Need easy machining and high conductivity, little strength? Tellurium copper C14500.
- Need conductivity and strength at temperature? Chromium copper C18200, or chromium-zirconium copper C18150 for the hottest duty. Cast parts: C81500 / CC140C.
- Need higher strength and can accept about half the conductivity? C17510 or C17500 (Class 3), or cast C82000.
- Need maximum strength, springiness or non-sparking properties? C17200 wrought or C82500 cast.
- Want to avoid beryllium? C18150 or C64700 cover many of the same applications.
Equivalents across standards
| USA | EN | DIN | BS | JIS |
|---|---|---|---|---|
| C14500 | CW118C CuTeP | 2.1546 | C109 | — |
| C15000 | CW120C CuZr | 2.1580 | — | — |
| C18200 | CW105C CuCr1 | 2.1291 | CC101 | — |
| C18150 | CW106C CuCr1Zr | 2.1293 | CC102 | — |
| C17200 | CW101C CuBe2 | 2.1247 | CB101 | C1720 |
| C17500 | CW104C CuCo2Be | 2.1285 | C112 | — |
| C17510 | CW110C CuNi2Be | 2.0850 | — | — |
| C64700 | CW111C CuNi2Si | 2.0855 | — | — |
| C81500 (cast) | CC140C CuCr1-C | 2.1292 G-CuCrF35 | CC1-TF | — |
Design and machining tips
- State the heat-treated condition and a verification method — hardness (HRB or HB) and/or conductivity (% IACS) — on the drawing.
- Plan the machining sequence. Rough machining before ageing and finishing after is common for beryllium copper; ageing causes a small, predictable dimensional change.
- Keep sections even in castings so the solution quench is effective through the whole part.
- Use sharp carbide tooling for aged beryllium and chromium copper; tellurium copper machines nearly as freely as free-cutting brass.
- Do not weld or braze aged parts unless you accept local loss of strength; joining heat over-ages the alloy.
Common mistakes
- Ordering "chrome copper" without a condition. As-cast or annealed chromium copper is much weaker and less conductive than solution-treated and aged material.
- Using pure copper for welding electrodes. It mushrooms quickly; chromium or chromium-zirconium copper lasts far longer.
- Choosing C17200 for a conductor. At about 20–25% IACS it is a spring alloy, not a conductor. Use C17510 if you need beryllium-copper strength with conductivity.
- Forgetting beryllium health controls when parts will be machined or ground downstream.
- Treating HCC1 as an alloy. HCC1 is the BS designation for high-conductivity cast copper, not a chromium copper; it appears here only as a cross-reference.
Heat treatment makes the difference
High-copper alloys such as beryllium copper (C17200, C17510), chromium copper (C18200, CuCr1) and chromium-zirconium copper (C18150, CuCr1Zr) reach their properties through solution treatment and age hardening. In the solution-treated state they are soft and easy to machine or form; after aging they become much harder and stronger while keeping high conductivity. Parts are often machined before aging and finished after. Drawings should state the final condition, hardness and minimum conductivity.
Before you send an enquiry
A short list of facts helps choose the right grade from this family and quote accurately the first time:
- The part and its job: what it does, what it touches, and what a failure would cost in downtime or safety.
- Service conditions: fluid or environment, temperature range, pressure, loads, speed and lubrication.
- Grade or standard on the drawing: the UNS, EN, BS, JIS, GB, DIN or IS designation, or the old grade name if that is all you have.
- Process or stock form: sand, centrifugal, continuous, gravity die or investment casting, or bar and plate. The most economical route can be suggested for your quantity.
- Machining stage: rough cast, semi-finished with allowance, or fully finished to drawing.
- Tests and documents: chemical analysis, mechanical and hardness tests, pressure test, NDT, material test certificate type (EN 10204 3.1), dimensional report and any third-party inspection.
- Quantities and timing: prototype, first batch, annual volume and delivery schedule.
- Market rules: any lead limit, drinking-water approval, RoHS or REACH requirement in the destination market.
With these details, the grade can be confirmed against the options covered on this page, or an equivalent suggested where it gives better value or performance for the same job.
Frequently asked questions
What is the best copper alloy for spot-welding electrodes?
Chromium-zirconium copper (C18150 / CW106C) is the most widely used RWMA Class 2 material for welding mild and coated steels. For higher-resistance materials such as stainless steel, Class 3 alloys like C17510 are common.
How strong is beryllium copper?
Fully aged C17200 typically reaches strengths above 1,000 MPa, making it the strongest copper alloy. The cast equivalent C82500 is also capable of very high strength after heat treatment.
Is chromium copper as conductive as pure copper?
No, but it is close. Aged chromium copper typically reaches around 75–85% IACS against about 100% for ETP copper, and it keeps its strength at temperatures where pure copper softens.
Can chromium copper be cast?
Yes. C81500, CC140C (CuCr1-C) and BS CC1-TF are cast grades. They must be solution treated and aged after casting to develop their properties.
Is beryllium copper dangerous?
Solid parts are safe to handle. Inhaling beryllium-containing dust or fume is hazardous, so machining, grinding and welding require extraction and proper controls.
What is tellurium copper used for?
Intricate machined electrical parts — terminals, connector pins, torch tips — where the part needs nearly pure-copper conductivity but must be machined efficiently.
What is a beryllium-free alternative to C17510?
Depending on the duty, chromium-zirconium copper (C18150) or the nickel-silicon Corson alloy (C64700) are often used. Compare conductivity, hardness and softening temperature for your application.
What should I specify when ordering high-copper castings?
Grade and standard, heat-treated condition, minimum hardness and/or conductivity, critical dimensions, machining requirements, quantity and the test documents you need, such as a material test certificate to EN 10204 3.1.
Send your drawing, get a quotation.
DWG, PDF, STEP or a sample photo — with quantity and destination port.